DISCLAIMER: The Graph Chatbot is not programmed to provide explicit or categorical answers to your questions. Rather, it transforms your questions into API requests that are distributed across the various IT services officially administered by EPFL. Its purpose is solely to collect and recommend relevant references to content that you can explore to help you answer your questions.
The title polymers of dialkenyldialkylammonium compds., useful in the coating and prepn. of paper, are prepd. in high space-time yield by the continuous or batch addn. of H2O-insol. azo compd. initiators in MeOH or DMF to aq. monomers. Thus, adding ten 2-mL portions of 0.01M methanolic AIBN [78-67-1] at 30 min intervals to 1 mol diallyldimethylammonium chloride as a 48% aq. soln. contg. 10 mg Chelaplex stirred at 80 Deg and stirring 90 min at 80 Deg gave a 96% conversion to a polymer [26062-79-3] with relative viscosity (1% NaCl) 1.85. [on SciFinder (R)]